Language
TRENARRU

+90 554 843 46 56 · yasin@brborline.com

PPRC Fusion Welding Times

Heating, joining and cooling times for Ø20–Ø110 mm PPRC socket fusion, based on DVS 2207-11 guide values.

Last reviewed: 21 Nov 2026

Key parameters

  • Heating tool temperature: 260 ± 10 °C.
  • Heating time starts once pipe and fitting are fully seated on the heating tool.
  • Below +5 °C ambient, increase the heating time by about 50%.
  • From Ø63 mm, use a suitable welding machine or bench.
  • Do not cool the joint with water or air.

Welding times chart

Table 1 – PPRC socket fusion, DVS 2207-11 guide values (SDR 11 and thicker-walled pipes). Insertion depth depends on the fitting socket; the range is taken from different manufacturer manuals.
Outside diameter d (mm)Insertion depth (mm)Heating (s), ambient ≥ +5 °CHeating (s), ambient < +5 °CJoining time, max (s)Hold fixed (s)Total cooling (min)
2014–14.558462
2515–167114102
3216.5–188126104
4018–20.512186204
5020–23.518276204
6324–27.524368306
7526–3030458306–8
9029–3340608406–8
11032.5–37507510508
  • For Ø75 and Ø90, the DVS table gives 6 min total cooling; some manufacturers recommend 8 min.
  • Joining time is the longest time left after removing the parts from the tool to join them and correct alignment; do not twist the parts.
  • Hold the joint fixed for the hold time and do not load it before the total cooling time has passed.

Socket welding step by step

  1. Cut the pipe square to its axis and deburr.
  2. Chamfer the pipe end at about 15° on the outside: about 2 mm up to Ø50, about 3 mm for larger sizes.
  3. Clean and dry the pipe end and the inside of the fitting; remove grease.
  4. Mark the insertion depth on the pipe.
  5. Check that the heating tool has reached 260 °C.
  6. Push the fitting fully onto the tool and the pipe into the tool up to the mark, without twisting, and wait for the heating time in the table.
  7. Pull both parts off the tool and join them at once, axially and without twisting.
  8. Hold the joint for the hold time, then wait for the total cooling time.

Common mistakes

  • Over-heating: molten material can bead inside the pipe and reduce the bore. Under-heating risks a weak fusion.
  • Twisting the parts while joining or pushing past the depth mark.
  • Welding wet, dusty or greasy surfaces.
  • Filling the line too early: one manufacturer manual recommends waiting at least 1 hour after the last weld.

Sources

Values were compiled from published documents based on the standards below and cross-checked against each other. Full standard texts are paid, so manufacturer catalogues declaring conformity to them were also used.

  1. DVS 2207-11 – Welding of thermoplastics, heated element welding of PP pipes (technical code preview, DVS)
  2. SIMONA – work.info Welding: heated element socket welding guide values, DVS 2207-1 and 2207-11
  3. aquatherm – Welding parameters, heated tool socket welding acc. to DVS 2207-11
  4. Uplast – PPRC pipe and fitting systems technical catalogue (wall thickness table S5–S2, application classes)
  5. Wavin – Pilsa piping systems technical and installation manual (support spacing, expansion, pressure test)

This page is for information only. The project specification, local regulations and the instructions of the pipe and fitting manufacturer always take precedence.

More technical pages

BORLINE PPRC pipes and fittings – Share sizes, SDR and packing needs for your export order and we will prepare a product list and quotation.

Get in Touch

Write to us about products, prices or dealership.